Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.

This is the free Material Data Center Datasheet of Ultramid® A3EG7 FC Aqua BK23285 - PA66-GF35 - BASF

Material Data Center offers the following functions for Ultramid® A3EG7 FC Aqua BK23285:
unit conversion, PDF datasheet print, comparison with other plastics, snap fit calculation, beam deflection calculation, parameters for material models, CAE Interfaces

Check here, which other Ultramid A datasheets, application examples or technical articles are available in Material Data Center

Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our disclaimer.
Product Texts
Ultramid® A3EG7FC Aqua black 23285 is optimized for plastic parts, mandatory requiring material approvals for drinking water or direct food contact
The product is approved according to
• 21 CFR FDA § 177.1500 "Nylon resins" (for repeated use applications only)
• 21 CFR FDA § 178.3297 "Colorants for polymers” (for repeated use applications only)
• European Food Contact European Food Contact Commission Regulation (EU) 10/2011
• GMP (EC) n°2023/2006

and provides the approvals for drinking water regulations of

• KTW
• DVGW W270
• WRAS
• ACS (disclosure of ingredients)
• NSF (disclosure of ingredients)

For questions regarding the compliance with further regulations, and certificates, please contact your local BASF representative or Plastics Safety (E-Mail: plastics.safety@basf.com).
Processing/Physical Characteristicsdry / condUnitTest Standard
ISO Data
Melt volume-flow rate, MVR 30 / * cm³/10min ISO 1133
Temperature 275 / * °C -
Load 5 / * kg -
Molding shrinkage, parallel 0.4 / * % ISO 294-4, 2577
Molding shrinkage, normal 1.0 / * % ISO 294-4, 2577
Mechanical propertiesdry / condUnitTest Standard
ISO Data
Tensile Modulus 11500 / 8500 MPa ISO 527
Stress at break 210 / 150 MPa ISO 527
Strain at break 3 / 5 % ISO 527
Tensile creep modulus, 1000h * / 6650 MPa ISO 899-1
Charpy impact strength, +23°C 95 / 105 kJ/m² ISO 179/1eU
Charpy impact strength, -30°C 75 / - kJ/m² ISO 179/1eU
Charpy notched impact strength, +23°C 14 / 22 kJ/m² ISO 179/1eA
Charpy notched impact strength, -30°C 12 / - kJ/m² ISO 179/1eA
Thermal propertiesdry / condUnitTest Standard
ISO Data
Melting temperature, 10°C/min 260 / * °C ISO 11357-1/-3
Temp. of deflection under load, 1.80 MPa 250 / * °C ISO 75-1/-2
Temp. of deflection under load, 0.45 MPa 250 / * °C ISO 75-1/-2
Vicat softening temperature, B 250 / * °C ISO 306
Coeff. of linear therm. expansion, parallel 17.5 / * E-6/K ISO 11359-1/-2
Coeff. of linear therm. expansion, normal 65 / * E-6/K ISO 11359-1/-2
Burning Behav. at 1.5 mm nom. thickn. HB / * class IEC 60695-11-10
Thickness tested 1.6 / * mm -
Yellow Card available yes / * - -
Burning Behav. at thickness h HB / * class IEC 60695-11-10
Thickness tested 0.8 / * mm -
Yellow Card available yes / * - -
Oxygen index 24 / * % ISO 4589-1/-2
Electrical propertiesdry / condUnitTest Standard
ISO Data
Relative permittivity, 1MHz 3.5 / 5.7 - IEC 62631-2-1
Dissipation factor, 100Hz 200 / 3000 E-4 IEC 62631-2-1
Dissipation factor, 1MHz 200 / 1500 E-4 IEC 62631-2-1
Volume resistivity 1E13 / 1E10 Ohm*m IEC 62631-3-1
Surface resistivity * / 1E10 Ohm IEC 62631-3-2
Electric strength 39 / 37 kV/mm IEC 60243-1
Comparative tracking index - / 550 - IEC 60112
Other propertiesdry / condUnitTest Standard
Water absorption 5 / * % Sim. to ISO 62
Humidity absorption 1.6 / * % Sim. to ISO 62
Density 1410 / - kg/m³ ISO 1183
Material specific propertiesdry / condUnitTest Standard
ISO Data
Viscosity number 145 / * cm³/g ISO 307, 1157, 1628
Diagrams
Viscosity-shear rate , Ultramid® A3EG7 FC Aqua BK23285, PA66-GF35, BASF
Shearstress-shear rate , Ultramid® A3EG7 FC Aqua BK23285, PA66-GF35, BASF
Dynamic Shear modulus-temperature , Ultramid® A3EG7 FC Aqua BK23285 (dry), PA66-GF35, BASF
Dynamic Shear modulus-temperature , Ultramid® A3EG7 FC Aqua BK23285 (cond.), PA66-GF35, BASF
Stress-strain , Ultramid® A3EG7 FC Aqua BK23285 (dry), PA66-GF35, BASF
Stress-strain , Ultramid® A3EG7 FC Aqua BK23285 (cond.), PA66-GF35, BASF
Secant modulus-strain , Ultramid® A3EG7 FC Aqua BK23285 (dry), PA66-GF35, BASF
Secant modulus-strain , Ultramid® A3EG7 FC Aqua BK23285 (cond.), PA66-GF35, BASF
Stress-strain (isochronous) 23°C, Ultramid® A3EG7 FC Aqua BK23285 (cond.), PA66-GF35, BASF
Creep modulus-time 23°C, Ultramid® A3EG7 FC Aqua BK23285 (cond.), PA66-GF35, BASF
Creep curve 23°C, Ultramid® A3EG7 FC Aqua BK23285 (cond.), PA66-GF35, BASF
Stress-strain (isochronous) 60°C, Ultramid® A3EG7 FC Aqua BK23285 (dry), PA66-GF35, BASF
Creep modulus-time 60°C, Ultramid® A3EG7 FC Aqua BK23285 (dry), PA66-GF35, BASF
Creep curve 60°C, Ultramid® A3EG7 FC Aqua BK23285 (dry), PA66-GF35, BASF
Stress-strain (isochronous) 90°C, Ultramid® A3EG7 FC Aqua BK23285 (dry), PA66-GF35, BASF
Creep modulus-time 90°C, Ultramid® A3EG7 FC Aqua BK23285 (dry), PA66-GF35, BASF
Creep curve 90°C, Ultramid® A3EG7 FC Aqua BK23285 (dry), PA66-GF35, BASF
Stress-strain (isochronous) 120°C, Ultramid® A3EG7 FC Aqua BK23285 (dry), PA66-GF35, BASF
Creep modulus-time 120°C, Ultramid® A3EG7 FC Aqua BK23285 (dry), PA66-GF35, BASF
Creep curve 120°C, Ultramid® A3EG7 FC Aqua BK23285 (dry), PA66-GF35, BASF
Stress-strain (isochronous) 140°C, Ultramid® A3EG7 FC Aqua BK23285 (dry), PA66-GF35, BASF
Creep modulus-time 140°C, Ultramid® A3EG7 FC Aqua BK23285 (dry), PA66-GF35, BASF
Creep curve 140°C, Ultramid® A3EG7 FC Aqua BK23285 (dry), PA66-GF35, BASF
Specific volume-temperature (pvT) , Ultramid® A3EG7 FC Aqua BK23285, PA66-GF35, BASF
Tensile modulus-temperature , Ultramid® A3EG7 FC Aqua BK23285 (dry), PA66-GF35, BASF
Tensile modulus-temperature , Ultramid® A3EG7 FC Aqua BK23285 (cond.), PA66-GF35, BASF
Characteristics
Processing
Injection Molding
Delivery form
Pellets, Black
Additives
Lubricants, Release agent
Special Characteristics
Heat stabilized or stable to heat
Certifications
Food contact, Food approval 10/2011, Food approval FDA 21 CFR, Drinking water contact, Drinking water contact KTW, Drinking water contact DVGW W270, Drinking water contact NSF 61
Regional Availability
Other text information
Injection molding
PREPROCESSING
Pre/Post-processing, max. allowed water content: .15 %
Pre/Post-processing, Pre-drying, Temperature: 80 °C
Pre/Post-processing, Pre-drying, Time: 4 h

PROCESSING
injection molding, Melt temperature, range: 280 - 300 °C
injection molding, Melt temperature, recommended: 290 °C
injection molding, Mold temperature, range: 80 - 90 °C
injection molding, Mold temperature, recommended: 80 °C
injection molding, Dwell time, thermoplastics: 10 min
Disclaimer
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com


Material Data Center is provided by M-Base Engineering + Software GmbH. M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors. Any decision about the application of materials must be double checked with the producer of this material.

Additional information about this material, like producer contact address, etc. can be found at www.materialdatacenter.com. For access to this extra information a registration is requested. Free online registration is available.